Acetal is the default gear material for light-to-medium duty, and it is also the material most often mis-designed, because it looks like metal on a drawing and behaves nothing like it in service. The failures are rarely dramatic — a gear that ran fine on the bench starts to whine after the first humid month, teeth lose their crown, or the bore loosens its grip on the shaft. All three trace back to design decisions that are cheap to fix on paper and expensive to fix in a mould or a batch of cut parts. This note collects the numbers we end up quoting in most gear enquiries.
Module: start from tooth load, not from the metal drawing
Converting a steel gear to acetal is not a like-for-like substitution. Acetal’s allowable tooth bending stress is roughly one-tenth of steel’s, and its allowable contact stress is lower still, so a straight module-for-module swap usually under-designs the tooth root. Practical starting points for POM-C:
- Light duty, low speed (hand wheels, dampers, actuators): module 1 to 1.5 is fine, but keep face width at least 8 to 10 times module so the tooth is not a thin disc.
- Conveyor and packaging drives, moderate torque: module 2 to 3, face width 8 to 12 times module. This is the sweet spot where acetal gears last for years.
- Higher torque, low speed: module 4 and up. Above module 4, cast nylon or POM with a steel insert often wins economically, because the acetal gear becomes large and expensive to cut.
The rule that catches most first-time designs: face width should never be less than about six times module. A module 2 gear with 8 mm face width is fine; the same gear with 5 mm face width concentrates load at the tooth edge and wears a step into the flank within months.
Backlash: the moisture allowance nobody budgets
Acetal absorbs water. At 50 percent relative humidity it reaches about 0.8 percent moisture by weight, and a machined or moulded gear grows accordingly — roughly 0.4 to 0.6 percent on diameter. On a 100 mm pitch diameter gear that is 0.4 to 0.6 mm of growth, split between the two gears in mesh, and it all goes into reducing backlash. A gear pair cut at zero backlash on a dry day will bind in a humid workshop.
The working rule: specify circumferential backlash of at least 0.04 times module plus 0.005 times pitch diameter, and add a further allowance when the operating environment is humid or washed. In practice:
| Pitch diameter | Module 2 minimum backlash | Module 4 minimum backlash |
|---|---|---|
| 50 mm | 0.25 mm | 0.40 mm |
| 100 mm | 0.55 mm | 0.70 mm |
| 200 mm | 1.15 mm | 1.30 mm |
If the application cannot tolerate that much backlash — a positioning drive, for example — the honest answer is to change material rather than to cut it tight and hope. A low-moisture polymer with tighter allowable backlash is a design change; a zero-backlash acetal pair is a warranty claim waiting to happen.
Tooth form and profile corrections
Standard 20° involute works, but acetal benefits from a few adjustments that cost nothing on a hobbing or moulding program. Increase root fillet radius to the maximum the cutter allows: acetal is notch-sensitive and the root fillet is where bending fatigue starts. Reduce addendum slightly — 0.9 to 0.95 times module — to avoid tip interference once thermal and moisture growth are included. And specify tip chamfering or rounding: acetal’s machined edges chip, and a chipped tip is a stress raiser that starts a crack.
For gears that run against steel, a small amount of profile modification on the acetal member spreads contact away from the pitch line and reduces the classic pitch-line pitting that shows up in high-cycle acetal/steel pairs.
Hub, web and bore rules
Acetal is not steel, and hubs designed as if it were are the second most common failure. Keep hub wall thickness at 1.5 to 2 times the tooth height; thicker hubs shrink more than the rim during cooling and induce hoop stress that cracks the web. Web thickness should be 0.3 to 0.5 times face width, with generous fillets where web meets rim and hub.
The bore is the other weak point. A plain acetal bore on a steel shaft will creep and lose interference at temperature; either use a keyed or splined connection, or press in a metal insert. For light duty, a bore with a flat and a set screw against a flat works if the hub wall is thick enough — which is why the hub rule above is not optional. Where the gear runs at temperature above 60 °C, an insert is the reliable answer.
Pairing: steel pinion, acetal wheel
The standard pairing — steel pinion driving an acetal wheel — remains the best wear combination, provided the steel pinion is finished properly. Specify pinion surface roughness of Ra 0.8 or better and a hardness above 200 HB; a rough, soft pinion acts as a file and the acetal wheel wears visibly within weeks. Avoid acetal running against acetal except in lightly loaded, low-speed, identical-tooth cases; two acetal gears in mesh wear each other at roughly double the rate of an acetal/steel pair.
Lubrication is optional in many acetal drives but not harmful: a light grease reduces noise and extends life, and it also buffers the moisture-driven backlash change by keeping the flanks from fretting. For food equipment, use a food-grade lubricant or run dry and accept a shorter service interval.
Thermal and moisture growth, in one number
For a first-pass check, assume a machined acetal gear grows 0.5 percent on a critical diameter from dry to humid equilibrium, and add 0.1 percent for a 40 °C temperature rise above 20 °C. Over a 150 mm pitch diameter, that is roughly 0.9 mm of combined growth — enough to consume a nominal backlash entirely. Design the centre distance with this in mind: fixed-centre drives should be given a slightly larger backlash; adjustable or spring-loaded centres handle it naturally.
Questions from gear enquiries
Can I use a standard catalogue acetal gear for a small series? Yes for light duty, but check the catalogue backlash against the table above. Catalogue gears are usually cut to a general-purpose backlash that is fine indoors and too tight in a humid plant.
Does glass-filled acetal help? It raises stiffness and reduces thermal growth, but it also raises wear on the mating steel and makes the tooth more brittle at the root. For gears, unfilled POM-C is usually the better tribological choice; glass-filled grades belong in structural parts.
How do I verify a prototype before committing to a batch? Run the pair for a week at operating temperature and humidity, then measure backlash again. If backlash closes by more than half in a week, the design has no moisture allowance and will bind in service.